Standard

ASME SA209/SA209M

ASME SA209/SA209M T1, T1a, T1b is the standard applicable to seamless carbon-Molybdenum Alloy-Steel Boiler and Superheater Tubes.

ASME SA209/SA209M tubes shall be made by the seamless process and shall be either hot-finished or cold finished as specified.

ASME SA209/SA209M covers several grades of minimum- wall-thickness, seamless, carbon-molybdenum alloy-steel, boiler and superheater tubes.

ASME SA209/SA209M covers tubes 1⁄2 to 5 in. [12.7 to 127 mm] inclusive, in outside diameter and 0.035 to 0.500 in. [0.9 to 12.7 mm], inclusive, in minimum wall thickness.


Size: 12.7 to 127 mm.

Wall Thickness: 0.9 to 12.7mm.

Shape: Round.

Length: Single random length/ Double random length or as customer’s actual request.

Grade: T1, T1a, T1b.

ASME SA209/SA209M Specification for General Requirements for Ferritic Alloy Steel, Austenitic Alloy Steel, and Stain- less Steel Tubes.


Chemical Composition (%)

Grade

C

Si

Mn

P

S

Mo

Cr

T1

0.10-0.20

0.10-0.50

0.30-0.80

≤0.025

≤0.025

0.44-0.65

/

T1a

0.15-0.25

0.10-0.50

0.30-0.80

≤0.025

≤0.025

0.44-0.65

/

T1b

0.14max

0.10-0.50

0.30-0.80

≤0.025

≤0.025

0.44-0.65

/


Mechanical Properties

Tensile Requirements and Hardness

Mechanical Properties

Grade

Tensile

Yield

Elongation

Hardness

Strength (Mpa)

Strength (Mpa)

(%)

(HRB)

T1

≥380

≥205

≥30

≤80

T1a

≥365

≥195

≥30

≤81

T1b

≥415

≥220

≥30

≤77


Flattening Test – One flattening test shall be made on specimens from each end of one finished tube, not the one used for the flaring test, from each lot.

Flaring Test – One flaring test shall be made on specimens from each end of one finished tube, not the one used for the flattening test, from each lot.

We use cookies and other tracking technologies to improve your browsing experience on our website, to show you personalized content and targeted ads, to analyze our website traffic, and to understand where our visitors are coming from,This behavior is in compliance with the user consent policy.